Appendix 2 - Condensation Chamber Test
Clasification Society 2024 - Version 9.40
Statutory Documents - IMO Publications and Documents - Resolutions - Maritime Safety Committee - Resolution MSC.215(82) - Performance Standard for Protective Coatings for Dedicated Seawater Ballast Tanks in all Types of Ships and Double-Side Skin Spaces of Bulk Carriers - (Adopted on 8 December 2006) - Annex - Performance Standard for Protective Coatings for Dedicated Seawater Ballast Tanks in all Types of Ships and Double-Side Skin Spaces of Bulk Carriers - Annex 1 - Test Procedures for Coating Qualification for Dedicated Seawater Ballast Tank of all Types of Ships and Double-side Skin Spaces of Bulk Carriers - Appendix 2 - Condensation Chamber Test

Appendix 2 - Condensation Chamber Test

1 Test condition

 Condensation chamber test shall be conducted in accordance with applicable standards.footnote

  • .1 The exposure time is 180 days.

  • .2 There are to be 2 test panels.

  • .3 The size of each test panel is 150 mm x 150 mm x 3 mm. The panels are to be treated according to the Performance Standard, table 1, paragraphs 1, 2 and 3 and coating system applied according to table 1, paragraphs 1.4 and 1.5. Shop primer to be weathered for at least 2 months and cleaned by low pressure washing or other mild method. Blast sweep or high pressure washing, or other primer removal methods not to be used. Weathering method and extent shall take into consideration that the primer is to be the foundation for a 15 year target life system. To facilitate innovation, alternative preparation, coating systems and dry film thicknesses may be used when clearly defined.

  • .4 The reverse side of the test piece shall be painted appropriately, in order not to affect the test results.

Figure 2 Condensation chamber

2 Test results

 According to section 2 (except for 2.2.5 and 2.2.6) of appendix 1.

3 Acceptance criteria

  3.1 The test results based on section 2 shall satisfy the following criteria:

Item Acceptance criteria for epoxy-based systems applied according to table 1 of this Standard Acceptance criteria for alternative systems
Blisters on panel No blisters No blisters
Rust on panel Ri 0 (0%) Ri 0 (0%)
Number of pinholes 0 0
Adhesive failure > 3.5 MPa
Adhesive failure between substrate and coating or between coats for 60% or more of the areas.
> 5 MPa
Adhesive failure between substrate and coating or between coats for 60% or more of the areas.
Cohesive failure > 3 MPa
Cohesive failure in coating for 40% or more of the area.
> 5 MPa
Cohesive failure in coating for 40% or more of the area.

  3.2 Epoxy-based systems tested prior to the date of entry into force of this Standard shall satisfy only the criteria for blistering and rust in the table above.

  3.3 Epoxy-based systems tested when applied according to table 1 of this Standard shall satisfy the criteria for epoxy-based systems as indicated in the table above.

  3.4 Alternative systems not necessarily epoxy-based and/or not necessarily applied according to table 1 of this Standard shall satisfy the criteria for alternative systems as indicated in the table above.

4 Test report

 According to section 4 of appendix 1.


Copyright 2022 Clasifications Register Group Limited, International Maritime Organization, International Labour Organization or Maritime and Coastguard Agency. All rights reserved. Clasifications Register Group Limited, its affiliates and subsidiaries and their respective officers, employees or agents are, individually and collectively, referred to in this clause as 'Clasifications Register'. Clasifications Register assumes no responsibility and shall not be liable to any person for any loss, damage or expense caused by reliance on the information or advice in this document or howsoever provided, unless that person has signed a contract with the relevant Clasifications Register entity for the provision of this information or advice and in that case any responsibility or liability is exclusively on the terms and conditions set out in that contract.