4.4.1 Two shear
                                 test specimens and two tensile test specimens are to be taken from
                                 each end of each composite plate for tests to be made on the bond
                                 strength. One shear and one tensile test specimen from each end are
                                 to be tested at ambient temperature after heating to the maximum allowable
                                 interface temperature, see 
                                 Ch  8,  4.2 Manufacture 4.2.1; the other two specimens are to be tested without heat treatment.
                                 
                              
                              
                              
                            
                           
                           
                           
                           
                           
                           
                           
                              
                              
                              4.4.3 The shear
                                 and tensile strengths of all the test specimens are to comply with
                                 the requirements of the manufacturing specification.
                              
                              
                              
                            
                           
                           
                           
                              
                              
                              4.4.4 If either the shear or tensile strength of the bond is less than the
                                 specified minimum but not less than 70 per cent of the specified minimum, two additional
                                 shear and two tensile test specimens from each end of the composite plate are to be
                                 tested and, in addition, bend tests as described in Ch  8,  4.4 Mechanical tests 4.4.6 and Table 8.4.1 Bend tests on explosion bonded
                                    aluminium/steel composites are to be made. 
                              
                              
                              
                              
                              
                                 
                                  
                                 
                                 Figure 8.4.2 Ram tensile test
                               
                              
                              
                              
                              
                              
                                 Table 8.4.1 Bend tests on explosion bonded
                                       aluminium/steel composites
                                 
                                    
                                       
                                          | Type
                                             of test | Minimum
                                             bend, degrees | Diameter of former | 
                                       
                                          | Aluminium in tension | 90 | 3T | 
                                       
                                          | Steel in tension | 90 | 3T | 
                                       
                                          | Side bend | 90 | 6T | 
                                       
                                          | 
                                                
                                                
                                                Note 
                                                   T is the total thickness of the composite plate. 
                                                 | 
                                    
                                 
                                 
                               
                              
                              
                            
                           
                           
                           
                           
                           
                              
                              
                              4.4.5 If either
                                 the shear or tensile strength of the bond is less than 70 per cent
                                 of the specified minimum the cause is to be investigated. After evaluation
                                 of the results of this investigation, LR will consider the extent
                                 of composite plate which is to be rejected.